I have done alot of testing with this resin . The process is vacuum and pressure depending on the wood I am stabilizing. With vacuum at - 28.5 you can get 100% penetration of the resin. If a blank of spalted maple is 110 grms before stabilizing after it will be 285 - 315 grms . I have done several hundred 2 x 2 x 6" wood blanks with this process and have had no problems . Hope this answers your questions . Troy
|